Cabbirka Alxanka Sare 0.1mm Ni80Cr20 Ni70Cr30 Ni60Cr15 Karma Evanohm Nichrome Wire Ni35Cr20 ee Foornada Warshadaha

Sharaxaad Gaaban:

Nickel-chromium, nickel, ferrochrome alloy silig oo leh koronto heerkulka sare leh iska caabbinta oksaydhka, xoog sare, aan jilicsanayn iyo faa'iidooyin taxane ah. Marka la isticmaalo waqti dheer, nooca isku midka ah iyo dhererka joogtada ah waa mid aad u yar, sidaas darteed waa doorashada ugu fiican ee lagu soo saaro qaybo koronto oo tayo sare leh.


  • Garde:Ni35Cr20
  • Cabbirka:0.1mm
  • Qaabka:Silig
  • Isticmaalka:Foornada Warshadaha
  • Cufnaanta (g/cm³):7.9
  • Faahfaahinta Alaabta

    FAQ

    Tags Product

    Alaabta iska caabbinta korantada ayaa si weyn loogu dabaqaa kuleyliyeyaasha korantada, gaar ahaan NiCr. Nichrome waa nikkel iyo chromium alloy taas oo inta badan loo isticmaalo soo saarista fiilada iska caabbinta sababtoo ah iska caabin sare oo sarreeya iyo sifooyinka anti-oxidation ee deggan heerkulka ilaa 1250 ° C waa sababta fiilooyinka iska caabbinta ay si fiican ugu habboon yihiin adeegga degaannada daran halkaasoo ay la kulmaan cadaadis iyo kulayl. Vladimir Plant of Precision Alloys waxa ay soo saartey alwaaxyo iska caabin ah iyo alwaaxyo kululaynta ka soo aasaaskeeda. Awoodeena waxay samaynaysaa fiilooyin, xariijimo, ribbon iyo foil, oo ay ku jiraan alliyada NiCr iyo Fe-Cr-Al alloys.

    Darajo

    Ni80Cr20

    Ni70Cr30

    Ni60Cr23

    Ni60Cr15

    Ni35Cr20

    Karma

    Evanohm

    Halabuurka magaca ah%

    Ni

    Bal

    Bal

    58.0-63.0

    55.0-61.0

    34.0-37.0

    Bal

    Bal

    Cr

    20.0-23.0

    28.0-31.0

    21.0-25.0

    15.0-18.0

    18.0-21.0

    19.0-21.5

    19.0-21.5

    Fe

    ≦1.0

    ≦1.0

    Bal

    Bal

    Bal

    2.0-3.0

    -

    Al1.0-1.7 Ti 0.3-0.5

    Al2.7-3.2 Mn0.5-1.5

    Al2.7-3.2 Cu2.0-3.0 Mn0.5-1.5

    Heerkulka shaqada ee ugu badan (°C)

    1200

    1250

    1150

    1150

    1100

    300

    400

    Resisability (Ω/cmf,20 ℃)

    1.09

    1.18

    1.21

    1.11

    1.04

    1.33

    1.33

    Resisability (uΩ/m,60°F)

    655

    704

    727

    668

    626

    800

    800

    Cufnaanta (g/cm³)

    8.4

    8.1

    8.4

    8.2

    7.9

    8.1

    8.1

    Heerarka kulka (KJ/m·h· ℃)

    60.3

    45.2

    45.2

    45.2

    43.8

    46.0

    46.0

    Iskuxidhka Balaadhinta Toosan×10¯6/℃)20-1000℃)

    18.0

    17.0

    17.0

    17.0

    19.0

    -

    -

    Meesha dhalaalaysa)

    1400

    1380

    1370

    1390

    1390

    1400

    1400

    Adag (Hv)

    180

    185

    185

    180

    180

    180

    180

    Xoogga Jiidka (N/mm2 )

    750

    875

    800

    750

    750

    780

    780

    Dheeraynta(%)

    20

    20

    20

    20

    20

    10-20

    10-20

    Qaab-dhismeedka Micrographic

    austenite

    austenite

    austenite

    austenite

    austenite

    austenite

    austenite

    Hantida Magnetic

    Maya

    Maya

    Maya

    Wax yar

    Maya

    Maya

    Maya

    Nolosha degdega ah (h/)

    81/1200

    50/1250

    81/1200

    81/1200

    81/1200

    -

    -